MIM 6061 |
Sintered state |
T6 |
Bar and sheet metal |
Vickers hardness HV |
50 ± 5 |
105 ± 5 |
86-110 |
Yield strength MPa |
78 |
296 |
55-245 |
Tensile strength MPa |
158 |
335 |
124-265 |
Elongation rate% |
26 |
6 |
25/8 |
Conductivity IACS |
41.9 |
\ |
47/43 |
Thermal conductivity coefficient W/(m2 K) |
136 |
\ |
180 |
Mirror polishing |
OK |
OK |
OK |
Salt mist |
48h |
\ |
OK |
PVD |
OK |
OK |
OK |
anodic oxidation |
OK |
OK |
OK |